产品参数
性能项目试验条件[状态]测试方法测试数据数据单位吸水量24小时浸渍ASTM D-5700.31%吸水量50%相对湿度ASTMD-5700.27%比重聽ASTM D-7921.39吸水量浸渍平衡点ASTM D-5700.75%模收缩聽聽1.7-1.9%挠曲变形强度23℃ASTMD-79070MPa洛氏硬度聽ASTM D-785117R scale线性热膨胀系数60~104℃ASTMD-69612.410-5m/m℃拉伸强度122℃ASTM D-638>16MPa挠曲系数100℃ASTMD-790690MPa挠曲系数23℃ASTM D-7902420MPa挠曲系数70℃ASTMD-7901260MPa抗剪强度23℃ASTM D-73249MPaIZOD冲击试验缺口-40℃ASTMD-256106j/m破裂点拉伸变形量122℃ASTM D-638>505%破裂点拉伸变形量-55℃ASTMD-63822%拉伸强度70℃ASTM D-638>38MPa负载变形量140kg/cm250℃ASTMD-6210.9%拉伸强度-55℃ASTM D-63899MPa挠曲系数-55℃ASTMD-7903670MPa拉伸强度100℃ASTM D-638>23MPa压缩应力23℃ 1%变形ASTMD-69516MPa抗拉伸冲击强度长试片23℃ASTM D-1822835kj/m2破裂点拉伸变形量23℃ASTMD-63891%挠曲疲劳忍耐限度50%RH 23℃ 106周期ASTM D-67125MPa弹性系数23℃ASTMD-6382330MPaIZOD冲击试验23℃ASTM D-256143j/m破裂点拉伸变形量100℃ASTMD-638>585%挠曲系数122℃ASTM D-790420MPa洛氏硬度聽ASTM D-78579Mscale破裂点拉伸变形量70℃ASTM D-638>545%压缩应力23℃ 10%变形ASTMD-69582MPa拉伸强度23℃ASTM D-63858MPa容积电阻率23℃ 0.2%含水量ASTMD-2572.3×1015Ω.cm介电因数50%RH 23℃ 106HzASTM D-1500.016
介电常数50%RH 23℃ 102~106HzASTM D-1503.6ohm-cm抗电弧3.1mmASTMD-495120sec介电强度瞬间Short time(2.3mm)ASTM D-14915.1(2.3)kv/mm熔点ASTMD-2133聽175℃自燃性聽UL-94HB
热畸变温度1.8MPaASTM D-64885℃线性热膨胀系数104~160℃ASTMD-69615.710-5m/m℃线性热膨胀系数29~60℃ASTM D-69612.010-5m/m℃热畸变温度0.5MPaASTMD-648174℃线性热膨胀系数-40~29℃ASTM D-69610.210-5m/m℃
(1)POM加工前可不用干燥,在加工过程中进行预热(80℃左右),对产品尺寸的稳定性有好处.
(2) POM的加工温度很窄(0~215℃),在炮筒内停留时间稍长或温度超过220℃时就会分解,产生刺激性强的甲醛气体.
(3) POM料注塑时保压压力要较大(与注射压力相近),以减少压力降.螺杆转速不能过高,残量要少;
(4) POM产品收缩率较大,易产生缩水或变形.POM比热大,模温高(80~100℃),产品脱模时很烫,需防止烫伤手指.
(5) POM宜在“中压、中速、低料温、较高模温”的条件下成型加工,精密制品成型时需用控制模温
(6)具高机械强度和刚性
(7)Zui高的疲劳强度
(8)环境抵抗性、耐有机溶剂性佳
(9)耐反覆冲击性强,良好的电气性质,复原性良好,具自已润滑性、耐磨性良好,尺寸安定性优.