%ASTM D570吸水率Equil.50%R.h.+73℉(+23℃)
%ASTM D570吸水率24hrs浸泡+73℉(+23℃)
%ASTM D570密度
g/cm³ASTM D792机械性能测试条件属性值单位测试方法摩擦系数+73℉(+23℃)静态
无无摩擦系数+73℉(+23℃)动态
无ThrustWasherTest3弹性系数+23℃
%ASTM D638弹性系数+73℉
%ASTM D638断裂伸长率+158℉(+70℃)
%ASTM D638断裂伸长率-68℉(-55℃)
%ASTM D638断裂伸长率+212℉(+100℃)
%ASTM D638断裂伸长率+73℉(+23℃)
%ASTM D638断裂伸长率+250℉(+122℃
%ASTM D638负荷变形2000psi@+122℉(14Mpa@50℃
%ASTM D621剪切强度+73℉
MPaASTM D732剪切强度+23℃
MPaASTM D732弯曲模量在25℃下+212℉
MPa无弯曲模量在25℃+122℃
MPa无弯曲模量在25℃下-68℉
MPa无弯曲模量在25℃下-55℃
MPa无弯曲模量在25℃下+70℃
MPa无弯曲模量在25℃下+250℉
MPa无弯曲模量在25℃下+73℉
MPa无弯曲模量在25℃下+23℃
MPa无弯曲模量在25℃下+100℃
MPa无弯曲模量在25℃下+158℉
MPa无拉伸屈服强度+122℃
MPaASTM D638拉伸屈服强度+212℉
MPaASTM D638拉伸屈服强度-55℃
MPaASTM D638拉伸屈服强度+100℃
MPaASTM D638拉伸屈服强度+23℃
MPaASTM D638拉伸屈服强度-68℉
MPaASTM D638拉伸屈服强度+158℉(+70℃)
MPaASTM D638拉伸屈服强度+70℃
MPaASTM D638拉伸屈服强度+73℉
MPaASTM D638拉伸屈服强度+250℉
MPaASTM D638弯曲模量+23℃
MPaASTM D790弯曲模量+73℉
MPaASTM D790疲劳极限+73℉
MPaASTM D671疲劳极限+23℃
MPaASTM D671压缩强度缩应力 +73°F@1%Def.
MPaASTM D695压缩强度+23℃@10%Def.
MPaASTM D695压缩强度+23℃@1%Def.
MPaASTM D695压缩强度+73°F@10%Def.
MPaASTM D695电气性能测试条件属性值单位测试方法绝缘穿击强度Short Time,90 mils
MV/mASTM D149体积电阻率+73°F(+23℃)0.2%H2O
ohms·mASTM D257绝缘穿击强度Short Time,2.3mm
MV/mASTM D149绝缘电阻系数 +73℉(+23℃)102to106Hz
无ASTM D150耗散因数+73℉(+23℃)106Hz
无ASTM D150耐电弧性120mil(3.1mm)
secASTM D495热性能测试条件属性值单位测试方法热变形温度1.8MPa
°CASTM D648热变形温度264psi
°FASTM D648热变形温度0.5Mpa
°CASTM D648热变形温度66psi
°FASTM D648导热系数
W/(K.m)无导热系数
W/(K.m)无熔点
°FASTM D2133熔点
°CASTM D2133线性膨胀系数+85 to +140℉
in/in/°FASTM D696线性膨胀系数+140 to +220℉
in/in/°FASTM D696线性膨胀系数-40 to +85℉
in/in/°FASTM D696线性膨胀系数-40 to +29℃
m/m/°CASTM D696线性膨胀系数+60 to +104℃
m/m/°CASTM D696线性膨胀系数+220 to +300℉
in/in/°FASTM D696线性膨胀系数+104 to +150℃
m/m/°CASTM D696线性膨胀系数+29 to +60℃
m/m/°CASTM D696冲击性能测试条件属性值单位测试方法简支梁冲击强度+23℃
无ASTM D256简支梁冲击强度40℃
无ASTM D256简支梁冲击强度-40℉
ft·lb/in²ASTM D256简支梁冲击强度+73℉
ft·lb/in²ASTM D256拉伸冲击+23℃
kJ/m²ASTM D1822拉伸冲击+73℉
kJ/m²ASTM D1822无缺口冲击强度+23℃
J/mASTM D256无缺口冲击强度+73℉
ft·lb/inASTM D256可燃性测试条件属性值单位测试方法UL 阻燃等级
无UL 94
硬度测试条件属性值单位测试方法洛氏硬度
无ASTM D785